1 Nisshin Steel Quality Products1 Nisshin Steel Quality Products
Foreword …………………………………………………2
Features …………………………………………………3
Production Process ……………………………………4
Characteristics and Applications ……………………5
Types of Stainless Steel Available …………………11
Available Sizes (SUS 304 and SUS 430) …………………13
Finish ……………………………………………………15
Surface-Treated Stainless Steel ……………………16
Dimensional Tolerances ……………………………17
Applications ……………………………………………20
Types of Protective Coatings ………………………25
Packaging ………………………………………………25
Coil Unit Weight Diagram ……………………………26
Information Needed to Meet Orders ………………………26
Contents
2Nisshin Steel Quality Products
Shunan Works
Nisshin Steel Co.,Ltd is an integrated steel manufacturer in Japan. Our products range
from ordinary steel to special steel, surface-treated products, stainless steel and welded
pipes and tubes. In 1958, we became the first Japanese producer of cold-rolled stainless
steel sheets in coil at Shunan Works and since then we have helped to make stainless
steel a material commonly used in the manufacturing of consumer durables both in Japan
and overseas.
Nisshin Steel has received wide acclaim as a supplier of cold-rolled sheets and strips and
hot bands of excellent quality. To meet the diversifying needs of our customers, we have
developed special types and grades of steel, including surface-treated products.
We are working to satisfy our customer's needs by providing a line of better products and
the quality of which is achieved through our use of advanced production facilities.
The following is an introduction to our stainless steel products, their applications and
other relevant information.
Foreword
3 Nisshin Steel Quality Products
Features
1
Nisshin products are manufactured by an integrated quality control process from melting to finishing.
Uniform Quality
2
The state-of-the-art production facilities offer high sheet thickness precision and flatness.
High Dimensional Precision and Flatness
3
Nisshin produces a wide variety of unique NSS type steel in addition to the JIS standard steels to meet any
needs of customers.
Nisshin products are given various types of surface finish.
Wide Variety of Types of Steel and Finish
4
Nisshin products widely ranges in thickness, length and width.
Wide Range of Sizes
5
Nisshin can give technical services suitable for user's needs,
making full use of our rich experience in the field of steel production.
Perfect After-Sales Service System
Converter Tandem Sendzimir cold rolling millHot strip mill (Kure Works)Continuous casting machine
4Nisshin Steel Quality Products
Production Process
Cr-ore, coke, Scrap,
and ferro-alloy
Hot strip mill
Cold-rolled strip (sheets)
Cold-rolled strip (coils)
Cold-rolled strip (coils)
Continuous annealing and pickling line
Continuous bright annealing line
Continuous annealing and pickling line
Coil grinding line
Ferritic type, martensitic type
Ferritic (single-phase), Austenitic type
Tandem Sendzimir mill
Sendzimir mill
Cluster mill
Bell type annealing furnace
Electric arc furnace L.D.converter Vacuum degassing vessel Continuous casting machine
Slab grinder Slab heating furnace
Skinpass mill
BA finish
No.2B finish
No.2D finish
Continuous shearing line
Coils
Slitting line
Tension leveling line
Finish polisher
Polished finish
Cold rolling process
Final process
Hot rolling process
Steel making process
・High crown controlled hot strip mill
・Tandem Sendzimir cold rolling mill
・Cold rolling by automatic gage controller
・Tension levelling line for strips and sheets
・Electronic automatic surface inspector
Strong points of manufacturing facility
6Nisshin Steel Quality Products5 Nisshin Steel Quality Products
Characteristics and Applications
1. Characteristics and Applications
■ Characteristics and Applications ■
Classification
Chemical Composition(%) Physical properties Mechanical properties
Nisshin
(NSS)
C Ni Cr Mo Others
Specific
gravity
g/cm3
Modulus of
elasticity
×103N/mm2
Average
modulus of
thermal
expansion
×10-6cm/cm/℃
20~100℃
Thermal
conductivity
W/m・℃
100℃
Tensile test Hardness test
Yield
strength
N/mm2
Tensile
strength
N/mm2
Elongation
%
HB HRB HV
Austenitic type
≦0.03 6.00~ 8.00 16.00~18.00 N≦0.20 7.93 194 16.9 16.3 ≧210 ≧530 ≧40 - ≦95 ≦218
≦0.15 6.00~ 8.00 16.00~18.00 7.93 194 16.9 16.3 ≧205 ≧520 ≧40 ≦187 ≦95 ≦218
≦0.08 8.00~10.50 18.00~20.00 7.93 194 17.3 16.3 ≧205 ≧520 ≧40 ≦187 ≦90 ≦200
304S ≦0.08 8.00~10.50 18.00~20.00 7.93 194 17.3 16.3 ≧205 ≧520 ≧40 ≦187 ≦90 ≦200
304ES ≦0.03 7.00~ 9.00 16.00~18.00 Cu:2.80~3.80 7.93 199 17.2 15.1 ≧155 ≧450 ≧40 ≦162 ≦90 ≦170
≦0.08 8.50~10.50 17.00~19.00 Cu:3.00~4.00 7.93 194 17.3 16.7 ≧155 ≧450 ≧40 ≦187 ≦90 ≦200
XM7 ≦0.05 8.50~10.00 18.00~20.00 Cu:2.50~4.00 7.93 194 17.3 16.7 ≧205 ≧510 ≧40 - ≦90 ≦200
304M2 ≦0.03 6.50~ 8.50 15.50~17.50 Cu:1.50~2.50 7.93 187 17.3 16.3 ≦335 ≦660 ≧50 - ≦86 ≦175
304M3 ≦0.06 6.40~ 8.00 15.00~17.00 Cu:1.50~2.50 7.93 187 17.3 16.3 ≧180 ≧500 ≧40 ≦187 ≦90 ≦200
≦0.03 9.00~13.00 18.00~20.00 7.93 194 17.3 16.3 ≧175 ≧480 ≧40 ≦187 ≦90 ≦200
≦0.08 7.00~10.50 18.00~20.00 N:0.10~0.25 7.93 194 16.9 16.3 ≧275 ≧550 ≧35 ≦95 ≦220
≦0.12 10.50~13.00 17.00~19.00 7.93 197 17.3 16.3 ≧175 ≧480 ≧40 - ≦90 ≦200
305M1 ≦0.08 11.00~13.00 15.00~17.00 Mn:2.00~4.00 7.93 194 17.3 16.3 ≧175 ≧480 ≧40 - ≦90 ≦200
302B ≦0.15 8.00~10.00 17.00~19.00 Si:2.00~3.00 7.93 194 16.2 15.8 ≧205 ≧520 ≧40 - ≦95 ≦220
ER-1 ≦0.07 12.00~13.50 18.50~20.00 Nb:0.05~0.20 Si:3.00~4.00 7.75 182 15.5 14.6 ≧255 ≧520 ≧45 - ≦95 ≦220
ER-4 ≦0.07 12.00~13.50 16.00~18.00 2.00~3.00 Si:2.00~3.00 7.85 182 14.5 - ≧205 ≧520 ≧40 - ≦95 ≦220
≦0.08 19.00~22.00 24.00~26.00 7.98 205 14.4 14.1 ≧205 ≧520 ≧40 ≦187 ≦90 ≦200
≦0.08 10.00~14.00 16.00~18.00 2.00~3.00 7.98 194 16.0 16.0 ≧205 ≧520 ≧40 ≦187 ≦90 ≦200
≦0.03 12.00~15.00 16.00~18.00 2.00~3.00 7.98 193 16.0 16.0 ≧175 ≧480 ≧40 ≦187 ≦90 ≦200
SCR ≦0.07 11.50~13.50 18.00~19.50 0.50~1.50 Cu:1.50~2.50 Si:2.50~4.00 7.75 194 16.7 16.0 ≧255 ≧520 ≧45 - ≦95 ≦220
AM-3 ≦0.08 8.50~10.00 18.00~20.00 Cu:3.60~4.50 7.93 193 - 16.5 ≧205 ≧510 ≧35 - - ≦200
Type
JIS
(SUS)
301
304
XM7
304L
304N1
305
302B
XM15J1
310S
316
316L
(315J2)
301L
8Nisshin Steel Quality Products
■ Characteristics and Applications ■
7 Nisshin Steel Quality Products
■ Characteristics and Applications ■
2. Characteristics and Applications
Classification
Chemical Composition(%) Physical properties Mechanical properties
Nisshin
(NSS)
C Ni Cr Mo Others
Specific
gravity
g/cm3
Modulus of
elasticity
×103N/mm2
Average
modulus of
thermal
expansion
×10-6cm/cm/℃
20~100℃
Thermal
conductivity
W/m・℃
100℃
Tensile test Hardness test
Yield
strength
N/mm2
Tensile
strength
N/mm2
Elongation
%
HB HRB HV
Ferritic type
≦0.08 10.50~11.75 Ti:6×C~0.75 7.75 194 10.8 23.8 ≧175 ≧300 ≧22 ≦167 ≦86 ≦175
445M2 ≦0.02 ≦0.60 21.00~23.00 1.00~1.50 N≦0.020 Ti:0.05~0.50 Nb:0.10~0.60 7.75 199 10.0 22.5 ≧205 ≧450 ≧22 ≦95 ≦220
410M1 ≦0.03 ≦0.60 11.50~13.50 7.75 202 9.9 23.8 ≧195 ≧360 ≧25 - ≦85 ≦170
HR-1 ≦0.03 ≦0.60 13.55~15.50 Si:0.70~1.50 Nb:0.20~0.80 7.75 211 11 21.9 ≧195 ≧360 ≧22 - ≦96 ≦230
NCA-1 ≦0.03 ≦0.60 17.00~19.00 Al:2.00~4.00 Ti≦0.50 7.35 201 10.0 18.8 - ≧490 ≧20 - ≦95 ≦220
NCA-2 ≦0.05 ≦0.60 11.50~13.50 Al:0.50~2.00 Si:1.00~2.00 Ti≦0.30 7.65 201 10.0 23.8 - ≧490 ≧20 - ≦95 ≦220
≦0.15 ≦0.60 11.50~13.00 7.75 202 9.9 23.8 ≧205 ≧440 ≧20 ≦200 ≦93 ≦210
≦0.15 ≦0.60 11.50~13.50 7.75 202 9.9 23.8 ≧205 ≧440 ≧20 ≦200 ≦93 ≦210
≦0.08 ≦0.60 11.50~13.50 7.75 202 9.9 23.8 ≧205 ≧410 ≧20 ≦183 ≦88 ≦200
410M4 0.04~0.10 ≦0.60 11.50~13.50 Si:0.10~0.40 Mn:0.50~1.00 7.75 202 9.9 23.8 ≧205 ≧410 ≧20 ≦88 ≦200
410M5 0.03~0.06 ≦0.60 11.50~12.10 ≦0.50 Cu:0.70~0.90 7.75 203 10.1 24.3 ≧205 ≧410 ≧20 ≦88 ≦200
0.16~0.25 ≦0.60 12.00~14.00 7.75 202 10.3 23.8 ≧225 ≧520 ≧18 ≦223 ≦97 ≦234
0.26~0.40 ≦0.60 12.00~14.00 7.75 202 10.3 23.8 ≧225 ≧540 ≧18 ≦235 ≦99 ≦247
WR-1 0.20~0.40 ≦0.50 12.00~14.00 Nb:0.30~0.50 7.70 201 10.3 24.9 ≧225 ≧540 ≧18 - - ≦247
HT980 0.03~0.06 3.00~5.00 12.00~14.00 Ti:0.15~0.50 7.75 203 10.8 20.5 ≧735 ≧880 ≧3 - - ≧290
HT1770 ≦0.09 6.50~7.75 13.50~15.50 Si:1.00~2.00 Cu:0.40~1.00 Ti:0.20~0.65 7.75 207 10.9 24.9 1000~1200 1100~1800 ≧3 - - 300~500
HT1770M ≦0.09 6.50~7.75 13.00~14.50 0.70~1.20 Si:1.00~2.00 Cu:0.40~1.00 Ti:0.20~0.65 7.75 207 10.9 24.9 1000~1200 1100~1800 ≧3 - - 300~500
HT2000 0.05~0.10 7.80~8.80 13.00~14.00 1.80~2.70 Si:2.20~3.20 7.80 200 14.0 20.8 1600~2200 1700~2300 ≧1 - - 500~650
431DP2 ≦0.08 1.00~3.00 16.00~18.00 7.73 201 10.5 19.9 750~1200 1050~1300 ≧6 - - 340~400
Type
JIS
(SUS)
445J1
410L
403
410
410S
420J1
420J2
632J1
SUH409
409M1 ≦0.03 ≦0.50 10.50~12.00 Ti:5×(C+N)~0.75 7.75 202 9.9 23.8 ≧195 ≧360 ≧25 - ≦85 ≦170
409M1S ≦0.03 ≦0.50 10.50~12.50 Si≦0.30 Ti:5×(C+N)~0.75 7.75 202 9.9 23.8 ≧175 ≧360 ≧25 ≦79 ≦150
405 ≦0.08 ≦0.60 11.50~14.50 Al:0.10~0.30 7.75 202 10.8 23.8 ≧175 ≧410 ≧20 ≦183 ≦88 ≦200
430 ≦0.12 ≦0.60 16.00~18.00 7.70 201 10.4 26.2 ≧205 ≧450 ≧22 ≦183 ≦88 ≦200
430LX 430M2 ≦0.05 ≦0.60 16.00~18.00 Ti:5×(C+N)~1.00 7.70 197 10.4 26.2 ≧175 ≧360 ≧28 - - ≦170
430LX 430M4 ≦0.03 ≦0.60 16.00~18.00 Nb:0.20~0.65 7.70 201 10.4 26.0 ≧205 ≧450 ≧22 - ≦88 ≦200
430M3 ≦0.04 ≦0.60 16.00~18.00 0.20~0.50 Ti:10×C~1.0 7.70 202 10.4 26.0 ≧205 ≧450 ≧22 - ≦88 ≦200
436L 436 ≦0.025 ≦0.60 17.00~19.00 0.50~1.50 N≦0.025 Ti:8×(C+N)~0.80 7.70 202 10.4 26.2 ≧205 ≧450 ≧22 ≦183 ≦88 ≦200
436J1L ≦0.025 ≦0.60 17.00~20.00 0.40~0.80 N≦0.025 Nb:8×(C+N)~0.80 7.70 ≧245 ≧410 ≧20 ≦90 ≦200
436J1L 432 ≦0.025 ≦0.60 17.00~19.00 0.45~0.65 N≦0.020 Nb:8×(C+N)~0.80 7.70 ≧205 ≧390 ≧25 - ≦170
430J1L 442M3 ≦0.03 ≦0.60 18.00~20.00 Cu:0.30~0.80 Nb:7×(C+N)+0.15~0.80 7.70 201 10.4 26.2 ≧205 ≧450 ≧22 - ≦88 ≦200
430J1L 442M3S ≦0.03 ≦0.60 18.00~20.00 Si≦0.50 Cu:0.30~0.80 Nb:7×(C+N)~0.80 7.75 201 10.4 26.2 ≧245 ≧410 ≧22 - ≦88 ≦200
444 444N ≦0.02 ≦0.60 17.50~20.00 1.75~2.50 N≦0.02 Nb:10×(C+N)~0.80 7.75 199 10.0 22.5 ≦205 ≧450 ≧22 - - ≦220
EM-2 ≦0.02 ≦0.60 17.50~20.00 1.75~2.50 Mn:0.70~1.50 Cu:0.10~0.30 7.75 206 9.9 21.9 ≦205 ≧450 ≧22 - - ≦220
Martensitic
type
High tensile
type
(including precipitation
hardening type)
Dual-phase type
9 Nisshin Steel Quality Products
■ Characteristics and Applications ■
3. Characteristics and Applications
Classification
Type
Characteristics ApplicationsJIS
(SUS)
Nisshin
(NSS)
Austenitic type
301L High strength can be obtained by skinpass. Highly resistant tointergranular corrosion. Railway rolling stock
301 High strength can be obtained by skinpass. Steel belts, metal gasket, springs
304 Typical austenitic stainless steel. Sundries, kitchen utensils, LNG tanks, others
304S Soft and amenable to deep drawing. Sundries
304ES Amenable to deep drawing, cold forging and shape freezing, etc. Deep drawing sensor case, flange
XM7 Cold working increased by adding copper to type 304. Sundries, Used for cold heading
XM7 Cold working increased by adding copper to type 304. Sundries, Used for cold heading
304M2 Amenable to deep drawing and stretch forming. Sundries, door knobs, sink bowls
304M3 Amenable to high speed bulging expanding. Gas burner parts
304L Lower carbon content than type 304, high resistance tointergranular corrosion. Oil refinery and papermaking equipment
304N1
Strength increased by adding nitrogen to type 304 while
keeping its ductility.
High strength material for construction,
colored fume pipe
305 Less work hardenability than type 304. Used for spinning, cold heading
305M3 High spring characteristics and high strength with no magnetism. Magnetic head cover
302B 302B More oxidation resistant than type 302, equal in oxidationresistance and strength with type 310S under 900。C. Automotive exhaust gas purifiers
(XM15J1) ER-1 Equal in oxidation resistance with type 309S (high qualityoxidation resistant steel).
Automotive exhaust gas purifiers, material
for burning part
ER-4
High temperature salt corrosion resistance and chloride
molten salt corrosion resistance.
Automotive flexible tube, incinerator
310S High quality oxidation resistant steel. Nitric acid tanks and burning chamber parts
316 Highly corrosion resistant. Slightly magnetized after forming. Chemical and paper industry equipmentand VTR guide rollers
316L Lower carbon content than type 316, highly resistant tointergranular corrosion.
Chemical, paper, dye and fertilizer industry
equipment
315J2 SCR
Resistant to stress corrosion cracking and has equal crevice
corrosion resistance with type 316.
Boilers and electric water heaters, indoor
plumbing
305M1 Extreme deep drawing is possible. Slightly magnetized after forming. TV electron guns and electronic parts
10Nisshin Steel Quality Products
■ Characteristics and Applications ■
4. Characteristics and Applications
Classification
Type
Characteristics ApplicationsJIS
(SUS)
Nisshin
(NSS)
Ferritic type
SUH409 Oxidation resistant steel developed by adding titanium to 11Cr type. Automotive parts and exhaust gas purifiers
445J1 Corrosion resistance increased by adding chromium to type 436L. Electronic portable water heater, roofing material
(445J1) 445M2 High corrosion and weather resistance Building materials
(410L) 410M1 Developed by reducing carbon content in type 410. Highly workable. Automotive exhaust gas purifiers and exhaust pipes
HR-1 High heat resistant 14Cr-Si-Mn-Nb Steel with high temperature strength and oxidation resistance. Automotive exhaust pipes
NCA-1 18Cr-Al Steel with high oxidation resistance. Oilstove burning columns which must heat red
NCA-2 13Cr-Si-Al Steel exhibiting high oxidation resistance. Oilstove burning columns
403 Developed by reducing silicon content in type 410. Valve sheets
410 Typical 13Cr stainless steel. Low quenching hardenability. Turbine blades, spoons, forks
410S Developed by reducing carbon content in type 410 to below 0.08%. High workability. Sundries and distillation column trays
410M4 Designed so that maximum Rockwell hardness of about 35 canbe obtained only by hardening in wide temperature range. Disk brakes
410M5 Shape stability after quench hardening increased by adding copper. Disk brakes
420J1 High quenching hardenability and work hardenability. Machine parts, table-knives
420J2 High quenching hardenability and work hardenability. Table-knives, slide calipers, rulers, scissors
WR-1
Strong resistance can be obtained against abrasive polishing
by hard grain.
Loom parts
HT980 High strength can be obtained by quench hardening at 750℃ or higher temperatures. Steel belts and high tension materials for welding
632J1 HT1770 Workable at low hardnesses because of high hardenabilityobtainable with age-hardening. High workability and long mold life. Seat sensor parts, punched springs
HT1770M High toughness, high strength and high fatigue strength can be obtained by adding molybdenum. Steel belts, golf club head
HT2000 High strength with ductility, toughness and fatigue strength. ID saw blades, flapper valve
431DP2
Spring characteristics can be obtained by a short-time age-
hardening.
Automotive parts, wrapping carrier, press
plate
409M1 Type 409 modified by increasing workability, oxidation resistance and high frequency weldability. Automotive exhaust pipes
409M1S Formability increased by reducing silicon content in type 409M1. Automotive exhaust pipes
405 Weldability and workability increased by adding aluminum to type 410. Oil refining distillation column trays
430 Typical ferritic stainless steel. Kitchen utensils, sundries, stove reflectors
(430LX) 430M2 Developed by adding titanium to type 430. Has higherworkability, weldability and corrosion resistance than type 430.
Sink bowls, burners, bicycle rims and bath
heater external plates
(430LX) 430M4 Developed by adding niobium to type 430 for increased workability and weldability. Bicycle rims and automotive parts such as wheel covers
430M3 Developed by adding molybdenum and titanium to type 430. High workability, weldability and corrosion resistance. Boilers
(436L) 436 More corrosion resistant than type 432 under the circumstance of dew condensation of exhaust gas. Material for automotive muffler
434 Developed by adding molybdenum to type 430. More corrosion resistant than type 430. Automotive trimmings
436J1L Developed by adding molybdenum and niobium to type 430, and highly reducing the carbon content and nitrogen content. Boilers, material for building interior and exterior
(436J1L) 432
Corrosion resistant under the circumstance of dew condensation
of exhaust gas and has better salt corrosion resistance.
Material for automotive muffler
442M3 Developed by adding copper and niobium to type 430. More corrosion resistant than type 434. Automotive trimmings, Automotive exhaust pipes
442M3S Formability increased by reducing silicon content in type 442M3. Automotive exhaust pipes
(444) 444N Free from stress corrosion cracking. Equal in corrosion resistance to type 316. Water reservoirs, heat reservoirs, solar heater collectors
EM-2 18Cr-2Mo-Mn-Nb Steel with high temperature strength and scale detachment resistance. Automotive exhaust pipes
Martensitic
type
High tensile
type
(including precipitation
hardening type)
Dual phase
type
11 Nisshin Steel Quality Products
Note�
Values adjacent to symbols ≦ and ≧ are chemical composition standard percentage.
Values adjacent to symbol = are chemical composition representative percentage.
Increase in carbon content
Increase in
carbon content Addition of niobium
Addition of copper
(Increased
high temperature
oxidation resistance)
Extremely
low carbon content
(Increased weldability
and workability)
(Increased weather resistance and intergranular corrosion resistance)
(Increased weldability and
intergranular corrossion resistance)
(Softening,
increased weldability)
Addition of aluminum
Low carbon content,
addition of silicon
and aluminum
Addition of titanium
(Workability, corrosion resistance
and weldability)
Extremely low carbon content, addition of molybdenum and titanium
(Increased pitting corrosion resistance
and intergranular corrosion resistance)
(Non-hardening,
increased weldability)
(Quench hardening
stability at low hardness)
Reduction in
silicon content
Reduction in
carbon content and
manganese content
Reduction in carbon content
Extremely low
carbon content
Low carbon content,
addition of titanium
Low carbon content, addition of niobium
Saving molybdenum, low carbon content, addition of copper and niobium
Extremely low carbon content,
addition of titanium
(Increased formability and
weldability)
Addition of niobium, reduction
in molybdenum content
(Increased formability and weldability)
Addition of molybdenum
Addition of manganese
(Increased high heat resistance and scale
detachment resistance)
(Increased age-hardenability and Introduction of spring characteristics)
(Increased
corrosion resistance)
(Increased formability)
Addition of nickel and titanium
Reduction in carbon and nitrogen content
(High strength and high toughness
after welding)
Addition of silicon
and copper
(Introduction of
precipitation hardenability)
(Increased hardenability and
wear resistance)
(Increased corrosion resistance
and formability)
Extremely low carbon
and nitrogen content,
increase in molybdenum content,
addition of niobium
Extremely low carbon
and nitrogen content,
increase in chromium content,
addition of molybdenum,
niobium and titanium
(Increased corrosion resistance,
weldability, and intergranular
corrosion resistance)
(Increased corrosion resistance,
weldability and intergranular
corrosion resistance)
Extremely low carbon content, addition of aluminum
(Increased high temperature oxidation resistance)
SUS410
SUS 420J 1
C=0.16~0.25
SUS 403
Si≦0.50
SUS 410S
C≦0.08
NSS HT 1770
15Cr-7Ni-0.7Cu-0.4Ti
NSS HT 980
12.5Cr - 4Ni-Ti
NSS 430M2
C=0.03 Ti = 7×(C+N)
NSS 430M3
C=0.01 Mo=0.4 Ti=0.55
NSS 444N
C, N≦0.02 Mo=2.0 Nb=0.4
NSS 442M3
19Cr-0.5Cu-0.5Nb
NSS 436
18Cr-1Mo-0.5Ti
NSS 432
18Cr-0.5Mo-0.4Nb
NSS 445M2
22Cr
本文档为【JIS SS】,请使用软件OFFICE或WPS软件打开。作品中的文字与图均可以修改和编辑,
图片更改请在作品中右键图片并更换,文字修改请直接点击文字进行修改,也可以新增和删除文档中的内容。
该文档来自用户分享,如有侵权行为请发邮件ishare@vip.sina.com联系网站客服,我们会及时删除。
[版权声明] 本站所有资料为用户分享产生,若发现您的权利被侵害,请联系客服邮件isharekefu@iask.cn,我们尽快处理。
本作品所展示的图片、画像、字体、音乐的版权可能需版权方额外授权,请谨慎使用。
网站提供的党政主题相关内容(国旗、国徽、党徽..)目的在于配合国家政策宣传,仅限个人学习分享使用,禁止用于任何广告和商用目的。